1.Choose the right timing. The first repair should be after 60-70 heats or when tapping time is no more than 2 minutes and 10 seconds, then repair after each 30-40 heats.
2.Incline the EAF after tapping, properly place the gunning sleeve in the taphole through sand filling hole.
3.Mount pallet on EBT handcart.
4.Mount nut cap on gunning sleeve.
5.Get the gunning mix ready on EBT platform.
6.Put the gunning head into sand filling hole to spry the gunning refractory material into the gap between gunning sleeve and taphole refractory bricks.
7.Close the gunning machine and pull out gunning head when the gunning material is in the same level with bottom material.
8.Dismount nut cap and pallet.
Article source:
The hot repair process of EAF taphole
E-mail:sales8@chinaelong.com
Henan Xinmi Changxing Refractory Material Co., Ltd. Located in Henan Province,China,has been making refractory products from 1978. ChangXing's product covers refractory materials,refractory brick, refractory castable,refractory nozzle, ceramic fiber, slide gate, etc; Changxing products have been exported to more than 20 countries, such as Thailand, Indonesia, Pakistan, Saudi Arabia, South Africa, Turkey, Iran, Iraq...